Aluman-16
Aluman-16 / AlMn1.6 (RHEINFELDEN ALLOYS) | High-pressure die and sand casting
Manufacturer-reported values. Do not use as certified design allowables. View sources ↗
| Temper | Wall | Yield MPa | Tensile MPa | Elong. % |
|---|---|---|---|---|
| F · High-pressure die casting | Not specified | 90–120 | 160–180 | 8–15 |
| F · Sand casting | Not specified | 80–100 | 130–160 | 4–8 |
F condition: Original-supplier performance range; wall thickness and test temperature not stated for this row.
Brinell hardness, F condition: 40–60 HBW
F condition: Original-supplier performance range; wall thickness and test temperature not stated for this row.
Brinell hardness, F condition: 40–50 HBW
Chemical composition
Only reviewed weight-percent bounds are listed. A blank bound means only the other threshold was reported.
Original-supplier Aluman-16, not all AlMn1.6 alloys. The 2015 overview, 2016 handbook, current product page and REACH sheet are one issuer, not independent votes. Main mechanical ranges do not specify wall thickness; they are not means or specification minima. REACH ingredient disclosure is not an ingot composition specification. Blank fatigue and gravity-shrinkage cells remain absent. Dust ignition does not describe bulk alloy ignition.
| Element / source label | Minimum wt% | Upper wt% |
|---|---|---|
| Si | — | 0.15 |
| Fe | 0.2 | 0.9 |
| Cu | — | 0.03 |
| Mn | 1.4 | 1.6 |
| Mg | — | 0.05 |
| Zn | — | 0.1 |
| Ti | — | 0.15 |
Physical and thermal properties
| Property | Reported value | Unit | Condition |
|---|---|---|---|
| density | 2.73 | kg/dm³ | Supplier approximate physical summary; temperature not specified |
| youngs modulus | 65–72 | GPa | Supplier physical summary; temperature not specified |
| thermal expansion | 24 | 10⁻⁶/K | Supplier physical summary; 20–200 °C |
| thermal conductivity | 1.5 | W/(K·cm) | Supplier physical summary; 20–200 °C |
| electrical conductivity | 20–26 | MS/m | Supplier physical summary; temperature not separately reported |
| electrical conductivity | 34.5–45 | %IACS | Supplier physical summary; temperature not separately reported |
| linear shrinkage | 1.2–1.5 | % | Sand casting; supplier physical summary |
| linear shrinkage | 0.8–1.2 | % | High-pressure die casting; supplier physical summary |
| melt solidification range | 645–660 | °C | Supplier melt and solidification summary; modification state not reported |
| density | 2.73 | g/cm³ | Manufacturer REACH technical information v2; at 20 °C; product form not further specified |
| melting range | 645–660 | °C | Manufacturer REACH technical information v2; measurement method not stated |
Processing properties
Source-reported comparisons, not certified limits.
| Property | Reported value |
|---|---|
| joining potential | can be hard soldered |
Additional property data
Source-reported values, specification intervals, minimums and strict bounds; an average is labeled only when the source reports it. Compare conditions before use.
| Property | Value | Condition |
|---|---|---|
| ignition temperature | 400 °C | Manufacturer REACH technical information v2; dust form only, not bulk alloy |
Evidence
Aluman-16 original-supplier handbook — RHEINFELDEN ALLOYS GmbH & Co. KG
Aluman-16 original-supplier overview — RHEINFELDEN ALLOYS GmbH & Co. KG
Aluman-16 original-supplier tdb — RHEINFELDEN ALLOYS GmbH & Co. KG
Show the exact source location for each value
- aluman-16-hpdc-f — PDF p. 58, Aluman-16 High-pressure die casting F detailed mechanical row ↗
- aluman-16-hpdc-f — PDF p. 3, Aluman-16 High-pressure die casting F mechanical summary ↗
- aluman-16-hpdc-f — PDF p. 79, Aluman-16 High-pressure die casting F mechanical summary ↗
- aluman-16-sand-f — PDF p. 58, Aluman-16 Sand casting F detailed mechanical row ↗
- aluman-16-sand-f — PDF p. 3, Aluman-16 Sand casting F mechanical summary ↗
- aluman-16-sand-f — PDF p. 79, Aluman-16 Sand casting F mechanical summary ↗
- Si — PDF p. 58, Aluman-16 Si composition ↗
- Si — PDF p. 77, Aluman-16 Si composition continuation ↗
- Fe — PDF p. 58, Aluman-16 Fe composition ↗
- Cu — PDF p. 58, Aluman-16 Cu composition ↗
- Cu — PDF p. 77, Aluman-16 Cu composition continuation ↗
- Mn — PDF p. 58, Aluman-16 Mn composition ↗
- Mg — PDF p. 58, Aluman-16 Mg composition ↗
- Mg — PDF p. 77, Aluman-16 Mg composition continuation ↗
- Zn — PDF p. 58, Aluman-16 Zn composition ↗
- Zn — PDF p. 77, Aluman-16 Zn composition continuation ↗
- Ti — PDF p. 58, Aluman-16 Ti composition ↗
- Ti — PDF p. 77, Aluman-16 Ti composition continuation ↗
- density — PDF p. 80, Aluman-16 density physical column ↗
- youngs modulus — PDF p. 80, Aluman-16 youngs_modulus physical column ↗
- thermal expansion — PDF p. 80, Aluman-16 thermal_expansion physical column ↗
- thermal conductivity — PDF p. 80, Aluman-16 thermal_conductivity physical column ↗
- electrical conductivity — PDF p. 81, Aluman-16 electrical_conductivity MS/m continuation ↗
- electrical conductivity — PDF p. 81, Aluman-16 electrical_conductivity IACS continuation ↗
- linear shrinkage — PDF p. 81, Aluman-16 linear_shrinkage Sand continuation ↗
- linear shrinkage — PDF p. 81, Aluman-16 linear_shrinkage High continuation ↗
- melt solidification range — PDF p. 81, Aluman-16 melt_solidification_range Melt continuation ↗
- density — PDF p. 4, Aluman-16 REACH density at 20 °C ↗
- melting range — PDF p. 3, Aluman-16 REACH melting range ↗
- joining potential — PDF p. 58, Aluman-16 distinguishing characteristics ↗
- ignition temperature — PDF p. 3, Aluman-16 REACH dust ignition temperature ↗