Silafont-36
AlSi10MnMg | High-pressure die casting
Manufacturer-reported values. Do not use as certified design allowables. View sources ↗
| Temper | Wall | Yield MPa | Tensile MPa | Elong. % |
|---|---|---|---|---|
| F | Not specified | 120–150 | 250–290 | 5–11 |
| T7 | Not specified | 120–170 | 200–240 | 15–20 |
Chemical composition
Reported weight-percent bounds. A blank lower bound means only an upper threshold was reported.
| Element / source label | Minimum wt% | Upper wt% |
|---|---|---|
| Si | 9.5 | 11.5 |
| Fe | — | 0.15 |
| Cu | — | 0.03 |
| Mn | 0.5 | 0.8 |
| Mg | 0.1 | 0.5 |
| Zn | — | 0.07 |
| Ti | 0.04 | 0.15 |
| Sr | 0.01 | 0.025 |
| P | — | 0.001 |
| others | — | 0.1 |
Physical and thermal properties
| Property | Reported value | Unit | Condition |
|---|---|---|---|
| young modulus | 74–83 | GPa | 20 °C |
| thermal expansion | 21 | 10⁻⁶/K | 20–200 °C |
| thermal conductivity | 1.5 | W/(K·cm) | temper O; 20–200 °C |
| electrical conductivity | 21–26 | MS/m | temper F; 20 °C |
| solidification range | 550–590 | °C | reported as 590–550 °C |
Fatigue
Source-reported fatigue values; conditions must be compared before use.
| Property | Value | Stress ratio | Cycles | Condition |
|---|---|---|---|---|
| Fatigue strength | 89 MPa | -1 | 50,000,000 | F |
Processing properties
Source-reported comparisons, not certified limits.
| Property | Reported value |
|---|---|
| heat treatment for property improvement | very good |
| hot crack tendency | low |
| sticking tendency | low |
| joining potential | high |
| die life | >80% |
| linear shrinkage | 0.4–0.6% |
Data under review
Density withheld: 2015 handbook and 2018 foldout report different densities; the foldout gives an approximate value without a temperature at this row.
Primary Aluminium Alloys for Pressure Die Casting ↗ — PDF p. 28, Physical composition, Density row
Aluminium Casting Alloys, 2018 foldout ↗ — PDF p. 9, Silafont-36 aligned physical-properties row
Evidence
Primary Aluminium Alloys for Pressure Die Casting — RHEINFELDEN ALLOYS
Show the exact source location for each value
- silafont-36-f — printed p. 8 / PDF p. 10, Silafont-36, F ↗
- silafont-36-t7 — printed p. 8 / PDF p. 10, Silafont-36, T7 ↗
- Si — PDF p. 28, Chemical composition ↗
- Fe — PDF p. 28, Chemical composition ↗
- Cu — PDF p. 28, Chemical composition ↗
- Mn — PDF p. 28, Chemical composition ↗
- Mg — PDF p. 28, Chemical composition ↗
- Zn — PDF p. 28, Chemical composition ↗
- Ti — PDF p. 28, Chemical composition ↗
- Sr — PDF p. 28, Chemical composition ↗
- P — PDF p. 28, Chemical composition ↗
- others — PDF p. 28, Chemical composition ↗
- young modulus — PDF p. 28, Physical composition ↗
- thermal expansion — PDF p. 28, Physical composition ↗
- thermal conductivity — PDF p. 28, Physical composition ↗
- electrical conductivity — PDF p. 28, Physical composition ↗
- solidification range — PDF p. 28, Physical composition ↗
- fatigue strength — PDF p. 28, Physical composition, Fatigue strength row ↗
- heat treatment for property improvement — PDF p. 28, Processing properties, Silafont-36 column ↗
- hot crack tendency — PDF p. 28, Processing properties, Silafont-36 column ↗
- sticking tendency — PDF p. 28, Processing properties, Silafont-36 column ↗
- joining potential — PDF p. 28, Processing properties, Silafont-36 column ↗
- die life — PDF p. 28, Processing properties, Silafont-36 column ↗
- linear shrinkage — PDF p. 28, Processing properties, Silafont-36 column ↗